    Diagram of reaction between HA and BDDE
    1. Diagram of reaction between HA and BDDE
    Appearance of composite hydrogels before and after autoclaving
    2. Appearance of composite hydrogels before and after autoclaving
    Appearance of composite hydrogels HAP45-1.0 with remained crosslinking reagents
    3. Appearance of composite hydrogels HAP45-1.0 with remained crosslinking reagents
    Storage modulus (a), loss modulus (b) and composite viscosity (c) of hydrogels before and after sterilization
    4. Storage modulus (a), loss modulus (b) and composite viscosity (c) of hydrogels before and after sterilization
    SEM morphologies of hydrogels
    5. SEM morphologies of hydrogels
    Push-out strain-stress curves of hydrogels
    6. Push-out strain-stress curves of hydrogels
    Swelling behavior of composite hydrogel HAP45-1.0 and stabilization in vitro
    7. Swelling behavior of composite hydrogel HAP45-1.0 and stabilization in vitro
    Enzymatic degradation of composite hydrogel HAP45-1.0 in vitro by HAase at 120 U/mL
    8. Enzymatic degradation of composite hydrogel HAP45-1.0 in vitro by HAase at 120 U/mL
    Fibroblast adhesion after being seeded on the surface of hydrogels observed by confocal fluorescence microscope
    9. Fibroblast adhesion after being seeded on the surface of hydrogels observed by confocal fluorescence microscope
    Proliferation of fibroblasts on surface of hydrogels (*p<0.05)
    10. Proliferation of fibroblasts on surface of hydrogels (*p<0.05)
    SampleHA/wt%HAP/wt%BDDE equivalent
    HA-1.01001.0
    HAP15-0.510150.5
    HAP30-0.510300.5
    HAP30-1.010301.0
    HAP45-1.010451.0
    Table 1. Amount of HA, HAP and BDDE in preparing composite hydrogels
    SampleBefore dialysisAfter dialysis
    HA/%HAP/%HA/%HAP/%
    HA-1.01002.01-
    HAP15-0.510151.582.38
    HAP30-0.510301.544.63
    HAP30-1.010302.197.73
    HAP45-1.010453.0015.8
    Table 2. Contents of HA and HAP in different composites before and after dialysis
    Ay0R2
    Mass swelling rate-51.6451.640.9992
    Volume swelling rate-78.8178.660.9984
    Table 3. The 1st order exponential decay equation fitting results of hydrogel HAP45-1.0 swelling behavior