• Journal of Inorganic Materials
  • Vol. 36, Issue 8, 877 (2021)
Yanqiu JING1、2, Qiang LIU2, Sha SU1、2, Xiaoying LI1, Ziyu LIU1, Jingya WANG1, and Jiang LI1、*
Author Affiliations
  • 11. Key Laboratory of Transparent Opto-Functional Inorganic Materials, Shanghai Institute of Ceramics, Chinese Academy of Sciences, Shanghai 201899, China
  • 22. School of Material Science and Engineering, Jiangsu University, Zhenjiang 212013, China; Center of Materials Science and Optoelectronics Engineering, University of Chinese Academy of Sciences, Beijing 100049, China
  • show less
    DOI: 10.15541/jim20200679 Cite this Article
    Yanqiu JING, Qiang LIU, Sha SU, Xiaoying LI, Ziyu LIU, Jingya WANG, Jiang LI. Fabrication of Highly Transparent Co:MgAl2O4 Ceramic Saturable Absorber for Passive Q-switching in 1.5 μm [J]. Journal of Inorganic Materials, 2021, 36(8): 877 Copy Citation Text show less

    Abstract

    The cobalt doped magnesium aluminum spinel is an efficient material for the passive Q-switching solid state lasers operating at the near infrared region. In order to prepare Co:MgAl2O4 transparent ceramics with high absorption cross section and high in-line transmittance, the cobalt doped magnesium aluminum spinel nanopowders with pure phase were synthesized via the co-precipitation method. And after vacuum sintering and hot isostatic pressing (HIP), highly transparent 0.05at% Co:MgAl2O4 ceramics were obtained. The influences of pre-sintering temperature on morphology and optical property of the Co:MgAl2O4 ceramics were studied. With the pre-sintering temperature increasing from 1500-1650 ℃, the relative density increased from 95.2% to 98.5%, while the relative density decreased to 97.7% with the pre-sintering temperature increasing to 1700 ℃. Because of the relative low density, the Co:MgAl2O4 ceramics were all opaque after vacuum pre-sintering. In the sintering temperature range of 1500-1700 ℃, the average grain size increased from 2.3 to 11.3 μm. After HIP post-treatment, the Co:MgAl2O4 ceramics pre-sintered from 1550 to 1700 ℃ were all transparent, the Co:MgAl2O4 ceramics pre-sintered at 1650 ℃ for 5 h and HIP post-treated at 1800 ℃ for 3 h showed the best optical quality, which were 81.4% at 400 nm and 85.9% at 900 nm, and the average grain size was 16.8 μm. The broad absorption bands in the wavelength range of 500-700 nm and 1200-1600 nm indicated that Co 2+ had incorporated into the spinel lattice. Moreover, the ground state absorption cross section of the best specimen is calculated with a value of 6.18×10-19 cm2 at 1540 nm, meaning that it’s a promising candidate for passive Q-switching in solid-state lasers.

    Co:MgAl2O4 is an efficient saturable absorber for passive Q-switching solid-state laser in eye safety laser. Co:MgAl2O4 single crystals produced by the Czochralski[1,2] or Verneuil[3] method were extensively reported[4,5,6]. However, polycrystalline Co:MgAl2O4 ceramics have attached much attention for its outstanding advantages over single crystals in the lower cost, higher doping level and scalable production.

    For transparent ceramics, the transparency depends largely on the numbers of optical scattering centers from secondary phase, grain boundaries and pores[7,8,9]. Generally, secondary phase can be reduced by controlling the composition of starting materials and the whole fabrication process. And the reflection and refraction in the grain boundary can be averted by choosing proper matrix materials without birefringence or other anisotropy. Therefore, cubic crystalline materials with high symmetry are usually used to prepare transparent ceramics. Many works have been devoted to the study on how to eliminate pores to the greatest extent. For the highly transparent Co:MgAl2O4 ceramics, the fully dense microstructure without pores is rather important. In general, transparent ceramics can be produced by pressure-assistant sintering methods[10,11,12]. Compared with pressureless sintering, pressure-assisted sintering can provide more driving force to eliminate pores and promote the densification of the ceramics[13], such as hot pressing (HP) and hot isostatic pressing (HIP). It is known that by using three dimensionally gas-assisted pressure, HIP shows much higher efficiency in fabricating dense ceramics with homogeneous microstructure in comparison to HP[11]. Most importantly, HIP post-treatment is an effective method to eliminate the close pores in ceramics by transmitting the external pressure in argon. And most of the open pores in green bodies can be removed by vacuum pre-sintering, thus the two-step sintering method of vacuum pre-sintering and HIP post-treatment is most popular and utilized. Additionally, ceramics pre-sintered with certain densities of 92%-95% have a better influence after HIP post-treatment[12]. Therefore, the pre-sintering mechanism of the Co:MgAl2O4 transparent ceramics should be systematically investigated to obtain the proper density for the HIP post-treatment.

    At present, many studies on the preparation of highly transparent Co:MgAl2O4 ceramics have been reported. Firstly, using AlF3 and MgF2 as sintering aids, Ikesue[13] fabricated highly transparent Co:MgAl2O4 ceramics through vacuum sintering and HIP post-treatment. However, the addition of a large number of additives might has a bad influence on the optical qualities due to the scatting centers formed by the secondary phases[14]. Goldstein, et al[15] and Luo, et al[16] obtained transparent Co:MgAl2O4 ceramics by a combination of vacuum sintering and HIP post-treatment without any sintering aids, while the optical quality of the ceramic was not good. In our previous work [17], transparent Co:MgAl2O4 ceramics with high optical quality were fabricated by lab-made Co:MgAl2O4 nanopowders. However, the influences of pre-sintering temperature on the quality of Co:MgAl2O4 ceramics were not investigated systematically. Thus, further research on Co:MgAl2O4 ceramics are urgently needed.

    In this study, the pure Co:MgAl2O4 nanopowders were synthesized by the co-precipitation method, and then transparent Co:MgAl2O4 ceramics were prepared by vacuum pre-sintering combined with sequent HIP post-treatment. This work provided a systematic investigation of the pre-sintering temperature on the densification, microstructure evaluation, and optical transparency of Co:MgAl2O4 ceramics. Meanwhile, absorption cross- section of the ceramic sample with best optical property was also discussed.

    1 Experimental

    The starting materials used were Mg(NO3)2·6H2O, Al(NO3)3·9H2O and Co(NO3)2·6H2O, and the ammonium carbonate was chosen as the precipitating agent. The detail procedure is similar with the previous work[17,18,19,20]. Firstly, the multi-cation solutions were obtained by dissolving the above nitrates with deionized water and the cationic stoichiometric ratio of Co:Mg:Al was set at 0.005:0.995:2. For the precipitation solution, the concentrati on of ammonium carbonate was 1.5 mol/L. Then, the precursor was obtained at room temperature by adding the mixed solution drop-wise into the precipitation solution at a speed of 4 mL/min under mild agitation. After agitating for half hour and aging for 1 h, the precursor precipitate was washed with deionized water and ethanol both for two times, following by drying at 70 ℃ for 48 h. Then the precursor was sieved with 200-mesh (74 μm) screen and calcined at 1100 ℃ for 4 h in air, and 0.05at% Co:MgAl2O4 nanopowders were obtained. Finally, the calcined powders were uniaxially dry-pressed into the pellet at 20 MPa followed by cold isostatically pressed at 250 MPa. After that, the green bodies were pre-sintered at 1500-1700 ℃ for 5 h in the tungsten mesh-heated vacuum furnace and HIP post- treatment at 1800 ℃ for 3 h in 200 MPa of argon. At last, the obtained Co:MgAl2O4 ceramics were mirror- polished to 1.2 mm in thickness.

    The field emission scanning electron microscope (FESEM, SU8220, Hitachi, Japan) was used to test the morphologies and microstructure of the powders and ceramics thermally etched at 1300 ℃ for 1 h. Grain sizes of the sintered samples were measured by the linear intercept method and the average grain size was calculated by multiplying the average linear intercept distance by 1.56[21]. The in-line transmittance and absorption coefficient of ceramics were measured with a UV-Vis-NIR spectrophotometer (Model Cary-5000, Varian, USA).

    2 Results and discussion

    The information of the as-synthesized precursor, including the XRD and FESEM results was presented in our previous report[17]. The FESEM micrograph of the Co:MgAl2O4 powders is displayed in Fig. 1. It can be seen that the calcined powders consist of near club-shaped particles and flaky particles with some holes, and the pores resulted from the decomposition of precursor.

    FESEM image of Co:MgAl2O4 powders

    Figure 1.FESEM image of Co:MgAl2O4 powders

    To observe the microstructures of obtained Co:MgAl2O4 ceramics, the samples were thermally etched at 1300 ℃ for 1 h. Fig. 2 shows the FESEM microstructures of Co:MgAl2O4 ceramics pre-sintered in vacuum at 1500- 1700 ℃ for 5 h. The ceramics show homogeneous structures, and no secondary phase existed. It can be noted that there are quite a few pores in the ceramics pre-sintered at 1500 and 1550 ℃ while the number of pores decreases obviously with the further increase of pre-sintering temperature, indicating the increase of the relative density. Notably, more pores can be found in the ceramic sample pre-sintered at 1700 ℃, and the phenomenon is consistent with the results reported in previous reports, which shows that many intragranular pores appear in the ceramics with high pre-sintering temperature[22]. These pores resulting from the high grain growth rate at high sintering temperatures[23] and are difficult to be eliminated by the following HIP post-treatment[24].

    FESEM images of Co:MgAl2O4 ceramics vacuum-sintered at different temperatures for 5 h(a) 1500 ℃; (b) 1550 ℃; (c) 1600 ℃; (d) 1650 ℃; (e) 1700 ℃

    Figure 2.FESEM images of Co:MgAl2O4 ceramics vacuum-sintered at different temperatures for 5 h (a) 1500 ℃; (b) 1550 ℃; (c) 1600 ℃; (d) 1650 ℃; (e) 1700 ℃

    The relative density and average grain size curves of the Co:MgAl2O4 ceramics pre-sintered at 1500-1700 ℃ as a function of sintering temperature are shown in Fig. 3. The average grain size increases with the increase of pre-sintering temperature while the relative density firstly increases and reaches the maximum at 1650 ℃. The decrease of the density is mainly caused by pores wrapped in grains or at grain boundaries. Moreover, the relative density of 98.5% at 1650 ℃ is still not enough to make the ceramics transparent. With the sintering temperature increasing, the average grain size of Co:MgAl2O4 ceramics calculated by the linear intercept method increase as expected, as shown in Fig. 3. A rapid grain growth occurs in the sintering temperature range of 1500-1700 ℃, the average grain size increases from 2.3 to 11.3 μm.

    Relative density and average grain size of 0.05at% Co:MgAl2O4 ceramics pre-sintered at different temperatures for 5 h

    Figure 3.Relative density and average grain size of 0.05at% Co:MgAl2O4 ceramics pre-sintered at different temperatures for 5 h

    The pre-sintered Co:MgAl2O4 ceramics were HIP post-treated at 1800 ℃ for 3 h to obtain fully dense ceramics. The microstructures of the thermally etched surfaces of the HIP post-treated samples are shown in Fig. 4. After the HIP post-treatment, no obvious pores can be found in ceramics pre-sintered at 1550-1700 ℃. However, for the sample pre-sintered at 1500 ℃ with HIP post-treatment, there are still some pores remained.

    FESEM microstructures of Co:MgAl2O4 ceramics vacuum-sintered at different temperatures for 5 h and then HIP post-treated at 1800 ℃ for 3 h(a) 1500 ℃; (b) 1550 ℃; (c) 1600 ℃; (d) 1650 ℃; (e) 1700 ℃

    Figure 4.FESEM microstructures of Co:MgAl2O4 ceramics vacuum-sintered at different temperatures for 5 h and then HIP post-treated at 1800 ℃ for 3 h (a) 1500 ℃; (b) 1550 ℃; (c) 1600 ℃; (d) 1650 ℃; (e) 1700 ℃

    Fig. 5 displays the average grain size of 0.05at% Co: MgAl2O4 ceramics pre-sintered at different temperatures for 5 h with HIP post-treatment. The grain grows greatly after HIP post-treatment and the average grain size of ceramics pre-sintered at 1500-1700 ℃ increases with the increasing pre-sintering temperature, which is 6.2, 12.3, 13.5, 16.8 and 20.3 μm, respectively.

    Average grain sizes of 0.05at% Co:MgAl2O4 ceramics pre-sintered at different temperatures for 5 h and then HIP post-treated

    Figure 5.Average grain sizes of 0.05at% Co:MgAl2O4 ceramics pre-sintered at different temperatures for 5 h and then HIP post-treated

    Fig. 6(a) shows the photo of mirror polished Co:MgAl2O4 ceramics pre-sintered at 1500-700 ℃ for 5 h and HIP post-treated at 1800 ℃ for 3 h with 200 MPa Ar atmosphere. It can be seen that all pre-sintered samples are opaque due to the low relative densities. After HIP post-treatment, the ceramic samples pre- sintered at the temperature above 1500 ℃ become transparent and the letters under the ceramics can be seen clearly, whereas the ceramic pre-sintered at 1500 ℃ with HIP post-treatment is still opaque. In addition, the blue color of the ceramics results from the absorption band of Co2+ at 500-700 nm. The in-line transmission 1500-1700 ℃ for 5 h and HIP post-treated at 1800 ℃ for 3 h is presented in Fig. 6(b). All transmission spectra of the ceramics pre-sintered at different temperatures show the similar features. The main absorption bands are located at 500-700 nm and 1200-1600 nm, which are the typical absorption bands of Co2+ ions located in tetrahedral Td sites[25,26]. Consistent with Fig. 6, the in-line transmittance of the sample pre-sintered at 1500 ℃ with HIP post-treatment is relatively low. In addition, the transmittance increases with the increase temperature of 1500-1650 ℃. The ceramic sample pre-sintered at 1650 ℃ shows the optimal optical transparency, with the transmittance of 81.4% at 400 nm and 85.9% at 900 nm, which is close to the theoretical transmittance. However, the transmittance of ceramics pre-sintered at 1700 ℃ decreases obviously. The theoretical transmittance can be calculated by the followed formula:

    ${{T}_{0}}=\frac{2n}{{{n}^{2}}+1}$

    where n is the refractive index of MgAl2O4 and it can be calculated by the Sellmeier equation[27]:

    $\frac{1}{{{n}^{2}}-1}=-\frac{A}{{{\lambda }^{2}}}+B$

    where λ is the wavelength of light, and A and B are equal to 0.0066 and 0.3659 μm 2, respectively. Thus the refractive index at 400 and 700 nm are 1.737 and 1.705, respectively, and the theoretical transmittance are calculated to be 86.5% and 87.3% at 400 and 900 nm. Moreover, the decrease of in-line transmittance within 200-400 nm wavelength can be found, meaning that there are still some nano-scale pores (less than 1 μm) [28] at the grain boundaries or entrapped in the grains as optical scattering centers in samples.

    Photo (a) and in-line transmission spectra (b) of the Co:MgAl2O4 ceramics pre-sintered at 1500-1700 ℃ for 5 h and HIP post-treated at 1800 ℃ for 3 hColorful figure are available on website

    Figure 6.Photo (a) and in-line transmission spectra (b) of the Co:MgAl2O4 ceramics pre-sintered at 1500-1700 ℃ for 5 h and HIP post-treated at 1800 ℃ for 3 h Colorful figure are available on website

    The absorption coefficient spectrum in 1000-1800 nm of 0.05at% Co:MgAl2O4 ceramic pre-sintered at 1650 ℃ and HIP post-treated at 1800 ℃ is shown in Fig. 7, which is the band intended to be used for the passive Q-switching in eye safe lasers. The broad absorption band in 1200-1600 nm is attributed to the transition from the4A2(4F9/2) ground-state to the 4T1(4F) excited multiplet. The absorption cross-section (σgas) is calculated by the following equations (3) and (4).

    ${{\sigma }_{\text{gas}}}=\frac{{{\alpha }_{\text{a}}}}{N}$
    $N=\frac{\rho \times {{N}_{\text{A}}}}{M}{{C}_{\text{S}}}$

    where σgas is the ground state absorption cross section, αa is the absorption coefficient, N is the concentration of Co2+ ions, NA is Avogadro’s number andM denotes relative molecular mass while CS is molar concentration of Co2+ in the ceramic. For the ceramics pre-sintered at 1650 ℃ and HIP post-treated at 1800 ℃, the value of αat 1540 nm is 4.68 cm-1. Thus the σgas is calculated to be 6.18×10-19 cm2, which is consistent with that of Co:MgAl2O4 transparent ceramics[18] and single crystal[2,3] reported in literatures, indicating its promising application for saturable absorber in 1.5 μm.

    Absorption coefficient spectrum of 0.05at% Co:MgAl2O4 ceramic pre-sintered at 1650 ℃ for 5 h and HIP post-treated at 1800 ℃ for 3 h

    Figure 7.Absorption coefficient spectrum of 0.05at% Co:MgAl2O4 ceramic pre-sintered at 1650 ℃ for 5 h and HIP post-treated at 1800 ℃ for 3 h

    3 Conclusion

    In this work, highly transparent 0.05at% Co:MgAl2O4 ceramics were fabricated from the co-precipitated Co:MgAl2O4 nanopowders by a combination of vacuum sintering at 1500-1700 ℃ for 5 h with hot isostatic pressing at 1800 ℃ for 3 h. The pure Co:MgAl2O4 nanopowders were obtained by calcining the precursor at 1100 ℃ for 4 h. The ceramics pre-sintered at 1500- 1700 ℃ are opaque because many intergranular pores were remained inside ceramics. The average grain sizes increase from 2.3 to 11.3 μm at the presintering temperature of 1500-1700 ℃. Pores located at grain boundary could be removed efficiently by hot isostatic pressing, which causes the relative density increasing. The in-line transmittance of the ceramic pre-sintered at 1650 ℃ for 5 h and HIP post-treated at 1800 ℃ for 3 h is close to the theoretical value, which are 81.4% at 400 nm and 85.9% at 900 nm. Besides, the ground absorption area is calculated to be 6.18×10 -19 cm2 at 1540 nm, and the high optical quality and σgas make it an attractive material in passive Q-switching at 1.5 μm.

    References

    [1] P JIANG D, Q ZOU Y, B SU L et al. A Co2+-doped alumina-rich Mg0.4Al2.4O4 spinel crystal as saturable absorber for a LD pumped Er:glass microchip laser at 1535 nm. Laser Physics Letters, 8, 343-348(2011).

    [2] V VOLK Y, M MALYAREVICH A, V YUMASHEV K et al. Anisotropy of nonlinear absorption in Co2+:MgAl2O4 crystal. Applied Physics B, 88, 443-447(2007).

    [3] V YUMASHEV K, A DENISOV I, N POSNOV N et al. Excited state absorption and passive Q-switch performance of Co2+ doped oxide crystals. Journal of Alloys and Compounds, 341, 366-370(2002).

    [4] Y LIN H, D SUN, N COPNER et al. Nd:GYSGG laser at 1331.6 nm passively Q-switched by a Co2+:MgAl2O4 crystal. Optical Materials, 69, 250-253(2017).

    [5] V YUMASHEV K. Saturable absorber Co2+:MgAl2O4 crystal for Q switching of 1.34-microm Nd3+:YAlO3 and 1.54-microm Er3+:glass Lasers. Applied Optics, 38, 6343-6346(1999).

    [6] V YUMASHEV K, A DENISOV I, N POSNOV N et al. Nonlinear absorption properties of Co2+:MgAl2O4 crystal. Applied Physics B-Lasers and Optics, 70, 179-184(2000).

    [7] Y LI X, Q LIU, W HU Z et al. Influence of ammonium hydrogen carbonate to metal ions molar ratio on co-precipitated nanopowders for TGG transparent ceramics. Journal of Inorganic Materials, 34, 791-797(2019).

    [8] H DAI Y, J LI, Y ZHANG et al. Preparation of Er,Yb:(LaLu)2O3 ceramic and its upconversion luminescent properties. Chinese Journal of Luminescence, 39, 488-493(2018).

    [9] B WEI J, G TOCI, A PIRRI et al. Fabrication and property of Yb:CaF2 laser ceramics from co-precipitated nanopowders. Journal of Inorganic Materials, 34, 1341-1348(2019).

    [10] H LEE S, R KUPP E, J STEVENSON A et al. Hot isostatic pressing of transparent Nd:YAG ceramics. Journal of the American Ceramic Society, 92, 1456-1463(2009).

    [11] L JIN L, H ZHOU G, S SHIMAI et al. ZrO2-doped Y2O3 transparent ceramics via slip casting and vacuum sintering. Journal of the European Ceramic Society, 30, 2139-2143(2010).

    [12] K ITATANI, T TSUJIMOTO, A KISHIMOTO. Thermal and optical properties of transparent magnesium oxide ceramics fabricated by post hot-isostatic pressing. Journal of the European Ceramic Society, 26, 639-645(2006).

    [13] A IKESUE. Transparent Spinel Ceramics, Method or Production Thereof, and Optical Meterial Using the Transparent Spinel Ceramics. European Patent(2008).

    [14] A IKESUE, L AUNG Y, T TAIRA et al. Progress in ceramic laser. Annual Review of Materials Research, 36, 397-429(2006).

    [15] A GOLDSTEIN, P LOIKO, Z BURSHTEIN et al. Development of saturable absorbers for laser passive Q-switching near 1.5 mm based on transparent ceramic Co2+:MgAl2O4. Journal of the American Ceramic Society, 99, 1324-1331(2016).

    [16] W LUO, P MA, F XIE T et al. Fabrication and spectroscopic properties of Co:MgAl2O4 transparent ceramics by the HIP post-treatment. Optical Materials, 69, 152-157(2017).

    [17] Q LIU, S SU, W HU Z et al. Fabrication and properties of Co:MgAl2O4 transparent ceramics for saturable absorber from co-precipitated nanopowder. Journal of the American Ceramic Society, 102, 3097-3102(2019).

    [18] S SU, Q LIU, W HU Z et al. A simple way to prepare Co:MgAl2O4 transparent ceramics for saturable absorber. Journal of Alloys and Compounds, 797, 1288-1294(2019).

    [19] G LI J, T IKEGAMI, H LEE J et al. Synthesis of Mg-Al spinel powder via precipitation using ammonium bicarbonate as the precipitant. Journal of the European Ceramic Society, 21, 139-148(2001).

    [20] A WAJLER, H TOMASZEWSKI, E DROŻDŻ-CIEŚLA et al. Study of magnesium aluminate spinel formation from carbonate precursors. Journal of the European Ceramic Society, 28, 2495-2500(2008).

    [21] I MENDELSON M. Average grain size in polycrystalline ceramics. Journal of the American Ceramic Society, 52, 443-446(1969).

    [22] L GAN, J PARK Y, H KIM et al. Effects of pre-sintering and annealing on the optical transmittance of Zr-doped Y2O3 transparent ceramics fabricated by vacuum sintering conjugated with post-hot-isostatic pressing. Ceramics International, 41, 9622-9627(2015).

    [23] M SEELEY Z, D KUNTZ J, J CHEREPY N et al. Transparent Lu2O3: Eu ceramics by sinter and HIP optimization. Optical Materials, 33, 1721-1726(2011).

    [24] F WANG S, J ZHANG, W LUO D et al. Transparent ceramics: processing, materials and applications. Progress in Solid State Chemistry, 41, 20-54(2013).

    [25] B CAMARGO M, D STULTZ R, M BIRNBAUM et al. Co2+:YSGG saturable absorber Q switch for infrared erbium lasers. Optics Letters, 20, 339-341(1995).

    [26] V VOLK Y, M MALYAREVICH V, V YUMASHEV K et al. Passive Q-switching of erbium glass laser by magnesium aluminosilicate sitall with cobalt ions. Journal of Applied Spectroscopy, 74, 140-146(2007).

    [27] R SHANNON, R SHANNON, O MEDENBACH et al. Refractive index and dispersion of fluorides and oxides. Journal of Physical and Chemical Reference Data, 31, 931-970(2002).

    [28] Z WANG Y, C LU T, L GONG et al. Light extinction by pores in AlON ceramics: the transmission properties. Journal of Physics D: Applied Physics, 43, 275403-275407(2010).

    Yanqiu JING, Qiang LIU, Sha SU, Xiaoying LI, Ziyu LIU, Jingya WANG, Jiang LI. Fabrication of Highly Transparent Co:MgAl2O4 Ceramic Saturable Absorber for Passive Q-switching in 1.5 μm [J]. Journal of Inorganic Materials, 2021, 36(8): 877